How to diagnose a bad print
When a print goes wrong, resist changing five things at once. Start with the symptom, think about which stage most likely caused it (stencil, press, ink, curing, fabric or registration), change one variable, and print another test. The sections below follow that order. Where a fix needs a step-by-step process, we link to a deeper guide.
Stencil problems
Pinholes (tiny dots of ink where there should be none). Common causes include dust or lint on the screen when you coated or exposed it, bubbles in the emulsion, poor degreasing, or emulsion that is too thin. Fixes: degrease and dry the screen well, work in a clean space, let mixed emulsion rest so air bubbles can rise, and coat more evenly. Block small pinholes on a finished screen with screen filler or a dab of emulsion. Our guide to coating a screen with emulsion covers coating technique.
Soft or breaking-down stencil edges. Often caused by underexposure, or a stencil that was not fully dry. Exposure times vary, so run a test as described in how long to expose screen printing emulsion.
Detail will not wash out, or the stencil looks hazy. This can come from overexposure, a film that is not dense enough, poor contact between film and screen, or emulsion that is too thick or was exposed to stray light. Improve film density (see making film positives), check contact, and retest exposure.
Ink leaking under the edges. Check that the edges of the stencil are sealed, the screen is taped where needed, and the off-contact is correct.
Press and technique problems
Blurry edges or ghosting. Possible causes include too little off-contact, too much squeegee pressure, a worn squeegee, a loose or low-tension screen, or ink that is too thin. Try adjusting off-contact so the screen peels away cleanly, use a sharp squeegee edge, reduce pressure, and slow down your stroke.
Streaks. A nicked squeegee blade, a rough platen, or lint or dried ink on the screen can cause streaks. Replace or resharpen the squeegee, clean the screen and check the platen surface.
Uneven or patchy coverage. Check the stroke pressure and angle, the flood stroke, ink amount and whether your mesh count and stencil thickness suit the ink. Patchy prints on textured or fuzzy fabric may need more ink deposit, a lower mesh count or a different blank.
Fibers or lint in the print. Use a lint roller on the shirt before printing. Some printers lightly flash the garment first.
Ink problems
Ink drying in the screen. More common with water-based inks, especially in dry or warm rooms. Keep the screen flooded between prints, and consider humidity control or retarder additives made for your ink. Shop owners sometimes use a fogger or steamer near the press to keep the air moist.
Ink bleeding or spreading at the edges. Ink that is too thin, too much pressure or too much ink on the screen can spread, especially on absorbent fabric.
Thin, translucent print. Too little ink deposit, a high mesh count, soft stencil, or too little squeegee pressure. On dark shirts, you may need an underbase, as described in screen printing white on black T-shirts.
Curing problems
Cracking, peeling or washing out. These are strong signs of under-curing, though very thick ink deposits or stretching during wear can also contribute. For plastisol, a common target is about 320°F (160°C) through the ink film. Check with an infrared thermometer or probe, adjust time and temperature, and always wash-test a sample before running a batch.
Scorched or shiny prints. Too much heat, or heat applied too long. Lower the temperature or shorten the dwell time.
Registration and fabric problems
Colors do not line up. Check registration marks, screen tension and whether the frames shift in the clamps. See how to register multi-color screen prints.
Dye bleed on dark or polyester shirts. Dye can migrate into white or light inks during curing. Low-bleed inks and lower cure temperatures can help; a test on the actual blank is wise.
Poor results on some fabrics. Smooth, tightly knit cotton generally prints more cleanly than loose, textured or stretchy fabrics. Waterproof, coated or highly stretchy synthetics can resist ink, so test first.
Symptom quick-reference table
| Symptom | Common causes | First things to try |
|---|---|---|
| Pinholes | Dust, bubbles, poor degreasing | Degrease, clean space, block holes |
| Blurry edges | Off-contact too low, too much pressure | Adjust off-contact, lighten pressure |
| Ghosting | Screen not peeling away, low tension | Increase off-contact, check tension |
| Streaks | Nicked squeegee, debris | Replace squeegee, clean screen |
| Patchy ink | Uneven pressure, textured fabric | Even stroke, more ink, test blank |
| Cracking | Under-cure | Check ink temperature and time |
| Washes out | Under-cure | Verify cure and wash-test |
| Misregistration | Marks off, loose screens | Recheck setup |
| Ink dries in screen | Low humidity, fast-drying ink | Keep flooded, humidify |
Keeping a test routine
Many defects are easier to catch before the real run. Print a test on scrap fabric, check the cure, wash-test a sample and keep a record of settings that work. Our list of screen printing tricks includes more habits that prevent reprints, and the full step-by-step guide shows where each step fits.